Importancia de la preparación de superficies
ferrosas en la protección de equipos e instalaciones industriales contra la corrosión
Prof. Xavier Figarella Gerente de Desarrollo Tecnológico
Universidad Metropolitana
![Page 2: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/2.jpg)
Propósito
Dar a conocer la importancia y alternativas en la preparación de superficies ferrosas en la protección de equipos e instalaciones industriales contra la corrosión.
![Page 3: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/3.jpg)
Contenido
• Corrosión electroquímica
• Preparación de superficies ferrosas
– Sandblasting
– Inhibidores de corrosión
– Convertidores de óxido
![Page 4: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/4.jpg)
Fe Fe+2(ac) + 2 e-
Fe´2(ac) Fe+3
(ac) + e-
Fe+2 Fe+3
Fe(OOH)
Metal
Herrumbre
Cátodo Ánodo O2 + 2 H2O + 4 e- 4 OH-
Agua O2 (Disuelto)
Corrosión Electroquímica
![Page 5: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/5.jpg)
Factores que aceleran el proceso de corrosión
• Presencia de electrolitos (sales solubles)
• Humedad ambiental
• Acidez del medio (pH)
• Temperatura
• Características de la superficie
• Otros
![Page 6: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/6.jpg)
Composición del herrumbre
• Geothita: Fe2O3.H2o • Lepidocrotita: Fe2O3.H2O
• Magnetita: Fe3O4
• Hidróxido Férrico : Fe(OH)3
![Page 7: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/7.jpg)
Influencia de la presencia de herrumbre en la corrosión
• El Herrumbre presenta muy poca adherencia a la superficie del metal y además es hidrófilo.
• El oxigeno disuelto en la humedad ambiental en contacto con el metal hace que continúe y se favorezca el proceso de corrosión:
![Page 8: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/8.jpg)
Importancia del control de la corrosión
En países industrializados, las pérdidas económicas a consecuencia de la corrosión alcanzan 3% del PIB. Para el caso de Panamá, esto representaría alrededor de 626 millones de dólares por año.
Lo anterior solo contempla las pérdidas estrictamente físicas y materiales. Esto no toma en consideración que la corrosión también acarrea problemas de seguridad industrial y de daños al ambiente, con pérdidas indirectas no ponderadas.
![Page 9: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/9.jpg)
Costos asociados
![Page 10: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/10.jpg)
Métodos de preparación de la superficie
• Métodos abrasivos (Sandblasting)
• Métodos químicos
– Inhibidores de corrosión
– Tratamientos ácidos
– Convertidores de óxido
![Page 11: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/11.jpg)
Sandblasting - Normas de Preparación de Superficies
• Normas Sandblasting
![Page 12: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/12.jpg)
Grados de Herrumbre
• Grados de herrumbre
![Page 13: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/13.jpg)
Limitaciones del Sandblasting Contaminación
![Page 14: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/14.jpg)
Limitaciones del Sandblasting Contaminación
![Page 15: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/15.jpg)
Limitaciones del Sandblasting Salud laboral
![Page 16: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/16.jpg)
Limitaciones del Sandblasting Salud Laboral
• Silicosis: es una enfermedad fibrósica-pulmonar de carácter irreversible y considerada enfermedad profesional incapacitante en muchos países.
La exposición intensa al sílice puede causar esta enfermedad en un año o menos, pero, por lo general, toma al menos 10 ó 15 años de exposición antes de que se presenten los síntomas. [Peters 1986; Ziskind et al. 1976].
la Administración de Seguridad y Salud Ocupacional (Occupational Safety and Health Administration, OSHA) ha establecido limitaciones al uso del Sandblasting.
![Page 17: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/17.jpg)
• Se preparan con una técnica conocida como “sandblasting”
• Consiste en aplicar un chorro de arena sobre la tela vaquera
• Se estima que cerca de 5.000 empleados están afectados de silicosis
Limitaciones del Sandblasting Salud Laboral
Preparar vaqueros desgastados causa decenas de muertes en varios países
![Page 18: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/18.jpg)
Limitaciones del Sandblasting Variables operacionales
La eficiencia del sandblasting depende de una serie de variables operacionales que deben ser estrictamente controladas para asegurar la productividad del proceso: • Tipo de boquilla • Diámetro y dureza del material abrasivo • Presión • Relación aire/abrasivo • Pericia del operario
![Page 19: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/19.jpg)
Limitaciones del Sandblasting Variables operacionales
• Ejemplo: Efecto del tamaño del abrasivo sobre el patrón de anclaje (grado de rugosidad que posee una
superficie)
![Page 20: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/20.jpg)
Inhibidores de Corrosión
Son compuestos químicos que se incorporan al medio corrosivo para retardar el proceso de corrosión.
• Condiciones que deben cumplirse:
1. Eficacia a bajas concentraciones
2. No modificar propiedades del medio
3. No tóxicos
4. Bajo costo
Los inhibidores de corrosión se clasifican como catódicos, anódicos o mixtos dependiendo de la reacción de corrosión que cada uno controla.
![Page 21: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/21.jpg)
Inhibidores de Corrosión
• Los inhibidores de corrosión más comunes son:
• Anódicos: molibdatos, ortofosfatos, nitritos, silicatos;
• Catódicos: zinc, polifosfatos, fosfonatos.
![Page 22: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/22.jpg)
Inhibidores de Corrosión Limitaciones
Los pretratamientos basados en diferentes ácidos minerales(Fosfatado) presentan serias limitaciones:
1. Las sales formadas en la interface metal / película usualmente generan abundante ampollamiento osmótico.
2. Además, en lo referente a las soluciones que incluyen
ácido ortofosfórico y fosfatos metálicos, no se alcanza una importante pasividad dado que la reacción con las diferentes capas de óxidos de hierro es marcadamente heterogénea.
![Page 23: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/23.jpg)
Ampollamiento Osmótico
• Lamina con ampollamiento
![Page 24: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/24.jpg)
¿Qué es un convertidor de óxido?
• El convertidor de óxido es un material que actúa químicamente transformando el herrumbre en compuestos inertes y estables, formando una barrera protectora contra la corrosión.
• Cuando la formulación incluye un copolímero biodegradable, el resultado es una doble capa de protección, inclusive antes del recubrimiento final.
![Page 25: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/25.jpg)
Convertidores de Óxido
• Rust converters are solutions or primers designed to be applied directly to a rusty surface to convert residual rust on steel surfaces to harmless and adherent chemical compounds.
• Unlike the standard scrape, prime, and paint regime, the user does not have to bring the surface down to bare metal. These in turn are able to develop a protective film Rust chemistry on the metal surface that protect against rust. http://events.nace.org/library/corrosion/MetalCoatings/rust-converter.asp
![Page 26: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/26.jpg)
Convertidores de Óxido Referencias
• Conversion of synthetic phase components of rust in aqueous solutions of oak tannin, of phosphoric acid, and of both these substances is described. The main components of atmospheric rust (viz., lepidocrocite, goethite, and magnetite) have been converted. Time of conversion ranged from 1 day to 12 months. The investigations were carried out using infrared spectroscopy.
• . Gust (1991) Application of Infrared Spectroscopy for Investigation of Rust Phase Component Conversion by Agents Containing Oak Tannin and Phosphoric Acid. Corrosion: June 1991, Vol. 47, No. 6, pp. 453-457. J. Gust (1991) Application of Infrared Spectroscopy for Investigation of Rust Phase Component Conversion by Agents Containing Oak Tannin and Phosphoric Acid. Corrosion: June 1991, Vol. 47, No. 6, pp. 453-457.
![Page 27: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/27.jpg)
c
• Use of Mössbauer Spectroscopy to Study Reaction Products of Polyphenols and Iron Compounds
• J. Gust 1, J. Suwalski 21Building Research Institute, Filtrowa 1,
00-950, Warsaw, Poland.
• 2Atomic Energy Institute, 05-400, Otwock-Swierk, Poland.
![Page 28: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/28.jpg)
Convertidores de Óxido Referencias
• Mössbauer spectroscopy was used to study parameters of the reaction products of iron compounds (FeIII) and polyphenols with hydroxyl (OH) groups in ortho positions. Polyphenols used in the reaction were catechol, pyrogallol, gallic acid, and oak tannin. The Fe-containing compounds were hydrated ferric sulfate (Fe2[SO4]3·nH2O), lepidocrocite (γ-FeOOH), goethite (α-FeOOH), magnetite (Fe3O4), and the carbon (C) steel corrosion products containing γ-FeOOH, α-FeOOH, and Fe3O4. Within a pH range of 1 to 7, all the polyphenols were shown to form with FeIII sparingly soluble complexes that were mixtures of mono- and bis-type complexes with different Mössbauer parameters. Parameters of each of the complex types were similar irrespective of the structure of the polyphenol used. A mixture of the mono- and bis-type complexes also formed as a result of a reaction between rust-phase components and oak tannin in an aqueous solution. When the reaction occurred on a surface of the rusted steel coated with an oak tannin solution, mainly mono-type complexes were formed. These complexes imparted anticorrosive properties to the converted rust.
![Page 29: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/29.jpg)
Convertidores de Óxido Referencias
Universidad de Panamá
“ Estudios de caracterización de productos de reacción entre materiales férreos y extractos acuoso de plantas”
Elizabeth Garcia de Sardaña.
Tesis de Maestría en Ciencias
Año 2000
![Page 30: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/30.jpg)
Convertidores de Oxido Mecanismo de Acción
• Diagrama de Pourbaix
![Page 31: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/31.jpg)
Comparación de Costos
• Sandblasting:
El costo aproximado está entre 30 y 35 $/ m2
• Tratamiento por convertidor de óxido:
El costo aproximado está entre 1 y 2 $ por m2, dependiendo del costo, rendimiento del convertidor y estado de la superficie.
![Page 32: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/32.jpg)
¿Qué es un convertidor de óxido?
• El convertidor de óxido es un material que actúa químicamente transformando el herrumbre en compuestos inertes y estables, formando una barrera protectora contra la corrosión.
• Cuando la formulación incluye un copolímero biodegradable, el resultado es una doble capa de protección, inclusive antes del recubrimiento final.
![Page 33: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/33.jpg)
¿Cómo se evalúa la eficiencia del método de preparación de la superficie?
• Poder Protector Total
El Poder Protector Total es una variable experimental que se evalúa a través del grado de ampollamiento y presencia de oxido en probetas que han sido sometidas a ensayos de corrosión acelerada según la normativa ASTM D-714-74.
Su variación con las horas de inmersión en cámara salina esta relacionada directamente con la frecuencia de los ciclos de mantenimiento. Se estima que cuando el poder protector total (PPT) alcanza al 40% se debe realizar un mantenimiento mayor. En el caso del Kill Ox los ensayos de laboratorio registran un período de 40.7 años
![Page 34: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/34.jpg)
Análisis Visual
![Page 35: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/35.jpg)
Poder Protector Total
Poder protector (PP) = Número de densidad(ND) * Número tamaño (NT) (PP)c = Poder protector en ampollamiento alrededor del corte (PP)a = Poder protector en ampollamiento al azar (MO)c = Manchas de oxido cercanas al corte (MO)a = Manchas de oxido al azar
PPT = (PP)c + (PP)a + (GH) + (MO)c + (MO)a % PPT = [PPT*100]/250
Ampollamiento:
Poder protector total:
![Page 36: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/36.jpg)
Las probetas (muestras) fueron sumergidas en una solución salina (NaCl al 5%) a 30oC, y evaluadas por un término de 500, 1000 y 1500 horas, a fines de determinar el Poder Protector Total (% PPT) y establecer una comparación de la efectividad pasivadora sobre superficies ferrosas del producto Kill Ox® comparado con la superficie preparada por el método de decapado mecánico con chorro de arena (sandblasting), y posteriormente tratadas con fondos epoxídicos, y pinturas alquídicas.
Pruebas de laboratorio
1 2 3 4
Laminas recubiertas con el convertidor, fondo y pintura. (1) Lamina original. (2) Con recubrimiento Kill OX® . (3)Con Fondo Epoxi. (4) Con
Pintura alquídica
![Page 37: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/37.jpg)
Prueba de Cámara salina ASTM B-117 Universidad Metropolitana Venezuela
Pruebas de laboratorio
![Page 38: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/38.jpg)
Resultados
0.00 20.00 40.00 60.00 80.00 100.00 120.00
0 horas
500 horas
1000 horas
1500 horas
Prob sin Kill Ox
Prob con Kill Ox
Comparación del % de PPT en probetas bajo prueba, con y sin Kill Ox en función del tiempo
![Page 39: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/39.jpg)
Resultados
70.00
75.00
80.00
85.00
90.00
95.00
100.00
0.00 0.50 1.00 1.50 2.00 2.50 3.00 3.50 4.00
Prob con Kill Ox Prob sin Kill Ox
Descenso del % PPT en función del tiempo en años
![Page 40: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/40.jpg)
Resultados
% PPT Años protección
Probeta con Kill Ox® 40,7
Probeta sin Kill Ox® 5,3
De acuerdo a las pruebas realizadas, se determino la siguiente relación máxima de Protección para llegar al 40% de PPT
![Page 41: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/41.jpg)
El Kill Ox® además de brindar un mayor poder protector total a la superficie, en términos de adhesión, demostró una perfecta compatibilidad entre los recubrimientos utilizados :
Acero - Kill Ox®
Kill Ox ® - Fondo epoxi
Fondo epoxi - acabado alquídico
1
2
3
Resultados
![Page 42: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/42.jpg)
Prueba de Planta: Petrobunker, Colón, Panamá
Prueba de campo
![Page 43: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/43.jpg)
Aplicación de pintura 24 h después
del curado final
Prueba de campo
![Page 44: Importancia de La Prep de Las Superficies](https://reader034.fdocuments.es/reader034/viewer/2022052315/54a1aa6eac7959b8248b47bf/html5/thumbnails/44.jpg)
Contactos
• VP Producción Especialidades: Eduardo Lander [email protected]
• Gerente Desarrollo Tecnológico: Xavier Figarella [email protected]
• Cel 62377645
• Teléfonos: 507 2038490/ 2038491
• www.ecotekgrp.com